Kajian Pengaruh Temperatur Aktivasi dengan Na OHTerhadap Karakter Karbon Aktif Mesopori Berbahan Dasar Limbah Kompleks Lumpur Industri Tekstil
ABSTRACT Textile sludge waste contains many organic matters so that it is potential to be used as mesoporous carbon precursor. Actived carbon with mesopore character is effective as adsorbentand catalyst carrier of large molecules. Synthesis of the activated mesoporous carbon was done with purpose t...
Saved in:
Main Author: | |
---|---|
Format: | Article NonPeerReviewed |
Published: |
[Yogyakarta] : Universitas Gadjah Mada
2008
|
Subjects: | |
Online Access: | https://repository.ugm.ac.id/27925/ http://i-lib.ugm.ac.id/jurnal/download.php?dataId=10988 |
Tags: |
Add Tag
No Tags, Be the first to tag this record!
|
Institution: | Universitas Gadjah Mada |
Summary: | ABSTRACT
Textile sludge waste contains many organic matters so that it is potential to be used as mesoporous carbon
precursor. Actived carbon with mesopore character is effective as adsorbentand catalyst carrier of large molecules.
Synthesis of the activated mesoporous carbon was done with purpose to study influence of activation temperature
toward chalC}ctersof the carbon. Process of the synthesis involved dry sludge (50 g) as precursor, concentrated
sodium silicate solution Si02 24.5% and Na20 7.5% (50 mL) as template source, 1 M HCI solution (50 mL) as
polimering agent, carbonization condition at 600 DC3 h under nitrogen.gas flow, activation conditions with NaOH
50% and various temperatures(400, 500, 600, 700, and 800 DC),and demineralizatin conditions with 0.1 M HCI
solution for 4 hand 125rpm. All of the products were characterizedwith methylen blue method to detennine specific
pore volumeand specific surface area. The carbon obtained at optimum temperature was characterizedagain with
surface area analyzer. Result of the research showed that the optimum condition was achieved at activation
temperatureof 500 DC.Characters of the synthesizedcarbon at the optimum condition were specific surface area of
638.32 m2/g,specific pore volume of 0.35 cm3/g,averagepore diameter of 21.78 A. and methylene blue number of
358.87 mg/g.
Keywords: actived mesoporous carbon, textile sludge, temperature |
---|