The optimization of heating temperature for carbon extraction from peat soil
This study aims to find the optimised heating temperature for carbon extraction from peat soil. Ccarbon from peat soil was extracted by the pyrolisation process at temperature, T = 200, 300, 400, 500, 600 and 700°C for 5 hours. The carbon, C and silica, Si content extracted from peat soil at v...
Saved in:
Main Authors: | , , , , |
---|---|
Format: | Conference or Workshop Item |
Language: | English |
Published: |
2017
|
Subjects: | |
Online Access: | http://eprints.uthm.edu.my/6972/1/P9685_e9b5eb0dd9117f7cb1f620801d11e299.pdf http://eprints.uthm.edu.my/6972/ https://doi.org/10.1088/1757-899X/298/1/012019 |
Tags: |
Add Tag
No Tags, Be the first to tag this record!
|
Institution: | Universiti Tun Hussein Onn Malaysia |
Language: | English |
Summary: | This study aims to find the optimised heating temperature for carbon extraction from
peat soil. Ccarbon from peat soil was extracted by the pyrolisation process at temperature, T =
200, 300, 400, 500, 600 and 700°C for 5 hours. The carbon, C and silica, Si content extracted
from peat soil at various heating temperatures were measured by using an Energy Dispersive
X-Ray analyzer (EDX) at 3 points on the sample surface. High atomic percentage of carbon
(95.44 %) was measured at T = 400°C, while the highest atomic percentage of silicon was
recorded at T = 700°C (30.79 %). The surface morphology of peat soil was analysed using
Scanning Electron Microscope (SEM) at 800 magnifying power, and it was clearly seen that
peat fragments were pyrolised at high heating temperature with pores enhancement. The
molecular structure parameter of the extracted carbon were identified using Laser Raman
analysis. The peak positions of D-band and G-band for raw peat soil were observed at Raman
shift of 1379.62 and 1549.02 cm-1, respectively. Meanwhile, the D-band for peat soil heated at
temperature of 400°C was 1391.56 cm-1 whereas the G-band has peak position at 1562.16 cm-1
.
From the Raman spectra of the optimum heating temperature at 400°C, it was revealed that the
carbon molecular structure from the peat soil is mainly attributed by graphite and diamond
structure. |
---|